Euronorme / Nom usuel |
W-nr | Din | Afnor | Aisi-ASTM | Bs | EN | Uni | UNF / UNS |
34CrMo4 / 34CrMoS4 / 35CrMo4 | 1.7220 / 1.7226 / 1.2330 | 34 Cr Mo 4 / 34 Cr Mo S 4 / 35 Cr Mo 4 | 34CD4 / 35CD4 / 38CD4 | 4130 / 4135 P20 / 4137 / AMS 6371 AMS 6346 | EN 19B / 708 A 30 / 708A30 / 708A37 (BP20) / 970 | 10083-3 / 10132-3 / 10250-3 .... | 34CrMo4KB / 35CrMo4 / 35CrMo4F | F.8331 / F.8231 / F.1250 / F.1254 / F125 |
NBN | SS | JIS | Gost | Appellation ® 1 | Appellation ® 2 | |||
34CRMO4 | 2234 | SCM432 / SCCrM3 / SCM435H (M) | AS38ChGM / 35ChM / 35ChML / 35XM | F65 / F 65 / KMT85 / UM7 | 35CrMo4 / V330 / 38CD4 |

Fiche technique
34CrMo4 / 34CrMoS4 / 35CrMo4
Retour à la liste
Appellations
Compositions
C | Si | Mn | P | S | Cr | Mo | |
---|---|---|---|---|---|---|---|
min | 0.300 | 0.600 | 0.020 | 0.900 | 0.150 | ||
moy | 0.400 | 0.750 | 0.025 | 0.035 | |||
max | 0.370 | 0.900 | 0.040 | 1.200 | 0.300 |
Applications et caractéristiques
Introduction
- 34CrMo4 / 34CrMoS4 / 35CrMo4
- ACIER D'AMELIORATION
- ACIER POUR TREMPE SUPERFICIELLE
- ACIER POUR L'EXTRUSION A FROID
A NOTER
- Livré à l'état adouci avec une dureté maximale en peau de 223 HB, sous forme de barres laminées et forgées.
- Très bonne aptitude au soudage et à l'oxycoupage.
- Formage à froid difficile nécessitant des machines et des lames très robustes.
- Usinage aisé.
GENERALITES
- Acier économique utilisé pour pièces de sections moyennes (ou grandes) soumises à de fortes contraintes.
- Acier de traitement thermique résistant bien aux chocs répétés et aux flexions alternées.
APPLICATIONS
- Engrenages,
- Crémaillères,
- Essieux,
- Porte-fusées,
- Arbres,
- Leviers,
- Crochets de traction,
- Vilebrequins et autres boulonnerie à haute résistance,
- Disques de turbines,
- Manivellles,
- Scie circulaire à chaud, etc...
PROPRIETES PHYSIQUES ET CARACTERISTIQUES MECANIQUES
Etat Traité :
1) Limite d'élasticité - Re :
- Jusqu'à 16 mm : ≥ 800 N/mm²
- De 17 à 40 mm : ≥ 650 N/mm²
- De 41 à 100 mm : ≥ 550 N/mm²
- De 101 à 160 mm : ≥ 500 N/mm²
2) Résistance à la traction - Rm :
- Jusqu'à 16 mm : 1000-1200 N/mm²
- De 17 à 40 mm : 900-1100 N/mm²
- De 41 à 100 mm : 800-950 N/mm²
- De 101 à 160 mm : 750-900 N/mm²
3) Allongement après rupture - A % :
- Jusqu'à 16mm : ≥ 11 %
- De 17à 40 mm : ≥ 12 %
- De 41à 100 mm : ≥ 14 %
- De 101 à 160 mm : ≥ 15 %
4) Striction à la rupture - Z :
- Jusqu'à 16 mm : ≥ 45 %
- De 17 à 40 mm : ≥ 50 %
- De 41 à 100 mm : ≥ 55 %
- De 101 à 160 mm : ≥ 55 %
5) Résilience - J :
- Jusqu'à 16 mm : ≥ 35 J
- De 17 à 40 mm : ≥ 40 J
- De 41 à 100 mm : ≥ 45 J
- De 101 à 160 mm : ≥ 45 J
TRAITEMENT THERMIQUE
1) Façonnage à chaud :
1100-850°C
2) Recuit d'adoucissement :
680-720°C
3) Normalisation :
850-890°C
4) Trempe :
830-870°C / Eau / Huile
5) Revenu :
540-680°C
6) Dureté Brinell HB :
223
DISTRIBUTEURS
- 34CrMo4 (DILLINGER) - (ESTANIT) - (HAECKERSTAHL) - (HAGENKOTTER) - (HAYES LEMMERZ)
- 34CrMo4 (ILSENBURGER GROBBLECH) - (WDI) - (ZAPP) - (HOESCH HOHENLIMBURG)
- 34CrMo4 / 34CrMoS4 (ASCOMETAL) - (VOMBOSTAHL) - (CORUS) - (EZM) - (GEORGSMARIENHUTTE) - (HAMMERWERK)
- 34CrMo4 / 34CrMoS4 (HEINE BEISSWENGER) - (KLÖCKNER) - (ORI MARTIN) - (OVAKO) - (PAULY STAHLHANDEL) - (SAARSTAHL) - (IMS FRANCE)
- 34CrMo4 / 34CrMoS4 (SCHMOLZ BICKENBACH) - (SALZGITTER) - (HERSTA) - (STAHLWERK ANNAHÜTTE) - (STAHLWERK UNNA MÜLLER)
- 34CrMo4 / 34CrMoS4 (FRIEDR. GUSTAV THEIS) - (STM STAHL) - (THYSSENKRUPP) - (VALLOUREC & MANNESMANN) - (VON MOOS STAHL)
- 34CrMo4 / 34CrMoS4 (SCHMIEDETECHNIK HAMMERWERK) - (WALZWERKE EINSAL)
- F65 (AUBERT & DUVAL)
- BGH 7220 - BGH 7226 (BGH EDELSTAHL)
- V 330 / V330 (BOHLER)
- Buderus 34CrMo4 / VCMo 135 (BUDERUS EDELSTAHL)
- DIRO-34CrMo4 -DIRO-34CrMoS4 (DIROSTAHL)
- 34CrMo4 / 34CrMoS4 / SCM 435 H (SUDWESTFALEN)
- THYROFORT 34CrMo4 - THYROFORT 34CrMoS4 (EWK - EDELSTAHL WITTEN KREFELD)
- 34CrMo4 / G34CrMo4 (GRODITZ)
- 1.7220 - 1.7226 (IMET) - (INTERSTAHL) - (KLEINEBERG) - (MALUGA) - (MWT MEYER) - (OBERSTE BEULMANN)
- 1.7220 - 1.7226 (PLATESTAHL) - (EDELSTAHL ROSSWAG) - (EDELSTAHL JPS) - (STAHL TEAM)
- PROCONS 7220 (PROMUNDO)
- CrMoll (SCANA)
- CR34M (HEROS)
- 34CrMo4 / 34CrMoS4 / GS-34CrMo4 (VOEST ALPINE)
- KMT85 / KMT 85 / UM7 / UM 7 (Ancienne appellation Ugine Service)
SPECIFICATIONS
- AMS 6370, AMS 6348, AMS-S-6758
- EN 10083-3 : Aciers pour trempe et revenu. Aciers alliés.
- EN 10132-3 : Feuillards laminés à froid pour traitement thermique. Aciers pour trempe et revenu.
- EN 10250-3 : Pièces forgées en acier pour usage général. Aciers spéciaux alliés.
- EN 10263-4 : Barres, fil machine et fils en acier pour transformation à froid et extrusion à froid. Aciers pour trempe et revenu.
- EN 10297-1 : Tubes ronds sans soudure en acier pour utilisation en mécanique générale et en construction mécanique.
- EN 1654-4 : Acier pour frappe et extrusion à froid. Aciers trempés et revenus.
- SEW 550 : Aciers pour pièces forgées lourdes.
- WL : Manuel des matériaux de l'aviation allemande.
Les indications et caractéristiques contenues dans cette fiche technique ne sont données
qu'à titre d'information afin d'aider le lecteur dans son évaluation personnelle. Elles ne
peuvent en aucun cas faire l'objet de garantie. Elles sont modifiables sans préavis en
fonction de l'évolution des techniques de fabrication et de la normalisation. Les valeurs
indiquées constituent des valeurs typiques ou moyennes et non des valeurs maximales ou
minimales garanties. La responsabilité de la SARL METONORM ne pourrait en aucun cas être
étendue au choix d'un produit ou aux conséquences de ce choix.